Process of chroming a car bonnet trim (continued)

<< Prev
Page 1
Page 2
Page 3
Page 4
Page 5
Page 6
>> Next

 |
 |
- The conductive wire and non-conductive weights are re-attached for the second electroplating.
|



- Pre-soak to remove polishing compounds (hot caustic 75°C) for 30 minutes.
|
 |
 |



 |
 |
- Alkali rinse.
|



- Electro-clean (cold cyanide solution) 12 volts anodic for 2 minutes.
|
 |
 |



 |
 |
- Rinse again.
|



- Acid etch (cold 10% sulphuric) for 2 minutes.
|
 |
 |



 |
 |
- Rinse again.
|



- Cyanide copper plate (hot cyanide 45°C) 12 volts cathodic 5 minutes.
|
 |
 |



 |
 |
- Rinse again.
|



- Acid etch (cold 10% sulphuric) 10 seconds.
|
 |
 |